Austenite series (Series 2, Series 3) |
Grade |
Chemical composition |
Unit :% |
|
JIS |
AISI |
DIN |
C |
Si |
Mn |
P |
S |
Ni |
Cr |
Mo |
Others |
Characteristics and Application |
SUS 201 |
201 |
– |
0.15 max |
1.00 max |
5.50 – 7.50 |
0.060 max |
0.030 max |
3.50 – 5.50 |
16.00 – 18.00 |
– |
N 0.25 max |
Alternative grade of SUS301 |
SUS 302 |
302 |
1.4319 |
0.15 max |
1.00 max |
2.00 max |
0.045 max |
0.030 max |
8.00 – 10.00 |
17.00 – 19.00 |
– |
|
Alternative grade of SUS302 |
SUS 303 |
303 |
1.4305 |
0.15 max |
1.00 max |
2.00 max |
0.20 max |
0.15 min |
8.00 – 10.00 |
17.00 – 19.00 |
(<0.60) |
|
Automatic machined parts such as screw, bolt |
SUS 303Se |
303Se |
– |
0.15 max |
1.00 max |
2.00 max |
0.20 max |
0.060 max |
8.00 – 10.00 |
17.00 – 19.00 |
– |
Se 0.15 min |
Screw |
SUS 303Cu |
– |
– |
0.15 max |
1.00 max |
3.00 max |
0.20 max |
0.15 min |
8.00 – 10.00 |
17.00 – 19.00 |
– |
Cu 1.50 – 3.50 |
Improved free cutting and cold heading quality, Shafts Usage |
SUS 304 |
304 |
1.4301 |
0.08 max |
1.00 max |
2.00 max |
0.045 max |
0.030 max |
8.00 – 10.00 |
18.00 – 20.00 |
– |
|
General corrosion resistance, food processing , equipment parts |
SUS 304L |
304L |
1.4306 |
0.030 max |
1.00 max |
2.00 max |
0.045 max |
0.030 max |
9.00 – 13.00 |
18.00 – 20.00 |
– |
|
To avoid intergranular corrosion (e.g. welding by SUS304) |
SUS 304N1 |
304N |
– |
0.08 max |
1.00 max |
2.50 max |
0.045 max |
0.030 max |
7.00 – 10.50 |
18.00 – 20.00 |
– |
N 0.10 – 0.25 |
Structural parts for higher strength |
SUS 304J3 |
– |
– |
0.08 max |
1.00 max |
2.00 max |
0.045 max |
0.030 max |
8.00 – 10.50 |
17.00 – 19.00 |
– |
Cu 1.00 – 3.00 |
Natural properties between 304 and XM-7,Bolts and Nuts Uasge |
SUS 305 |
305 |
– |
0.12 max |
1.00 max |
2.00 max |
0.045 max |
0.030 max |
10.50 – 13.00 |
17.00 – 19.00 |
– |
|
Low work hardening. Cold heading quality |
SUS 309S |
309S |
1.4833 |
0.08 max |
1.00 max |
2.00 max |
0.045 max |
0.030 max |
12.00 – 15.00 |
22.00 – 24.00 |
– |
|
Superior corrosion and oxidation resistance to 304, Parts for chemical plant., heat treatment, furnace |
SUS 310S |
310S |
1.4845 |
0.08 max |
1.50 max |
2.00 max |
0.045 max |
0.030 max |
19.00 – 22.00 |
24.00 – 26.00 |
– |
|
Superior corrosion and heat resistance to SUS309S. Parts for thermal exchanger in furnace. |
SUS 316 |
316 |
1.4401/1.4436 |
0.08 max |
1.00 max |
2.00 max |
0.045 max |
0.030 max |
10.00 – 14.00 |
16.00 – 18.00 |
2.00 – 3.00 |
|
More corrosion-resisting than 304. Anti-rust purpose . Chemical plant equipment(paper, soap, chemical textile, fertilizer) |
SUS 316L |
316L |
1.4404/1.4435 |
0.030 max |
1.00 max |
2.00 max |
0.045 max |
0.030 max |
12.00 – 15.00 |
16.00 – 18.00 |
2.00 – 3.00 |
|
Extreme low carbon 316. High anti-corrosion |
SUS 316F |
– |
– |
0.08 max |
1.00 max |
2.00 max |
0.045 max |
0.10 min |
10.00 -14.00 |
16.00 – 18.00 |
2.00 – 3.00 |
|
Enhanced free cutting quality by adding sulpur into 316. Watchband Usage |
SUS 317 |
317 |
1.4449 |
0.08 max |
1.00 max |
2.00 max |
0.045 max |
0.030 max |
11.00 – 15.00 |
18.00 – 20.00 |
3.00 – 4.00 |
|
Environment which requires corrosion resistance (e.g. dyeing machine) |
SUS 317L |
317L |
1.4438 |
0.030 max |
1.00 max |
2.00 max |
0.045 max |
0.030 max |
11.00 – 15.00 |
18.00 – 20.00 |
3.00 – 4.00 |
|
Improved intergranular corrosion resistance of SUS317 (e.g. dyeing machine) |
SUS 321 |
321 |
1.4541 |
0.08 max |
1.00 max |
2.00 max |
0.045 max |
0.030 max |
9.00 – 13.00 |
17.00 – 19.00 |
– |
Ti 5*C% min |
Ti addition. High temperature purpose. Parts which are unable to be heat treated after welding. equipment parts used between 730 900 thermal condition |
SUS 347 |
347 |
1.4550 |
0.08 max |
1.00 max |
2.00 max |
0.045 max |
0.030 max |
9.00 – 13.00 |
17.00 – 19.00 |
– |
Nb10*C% min |
Superior intergranular corrosion resistance |
SUS XM7 |
302HQ |
– |
0.08 max |
1.00 max |
2.00 max |
0.045 max |
0.030 max |
8.50 – 10.50 |
17.00 – 19.00 |
– |
Cu 3.00 – 4.00 |
Cu addition into 304. Enhanced cold heading quality |